COATING THICKNESS GUIDE

COATING THICKNESS GUIDE

HOW MUCH IS ENOUGH · HOW MUCH IS TOO MUCH
v2.3 · ISSUE 02.09.2026
REVIEW DUE 07.2028
REFERENCED BY EVERY GERMA-TECH TDS

Most of the jobs that come back are not failures of the paint. They are failures of quantity. Too many coats, too much product in each coat, and not enough time between them. This guide is the number, and the reason behind the number.

300 µm
The total film on a panel should not pass 300 microns.
That is every layer added together — epoxy, filler, primer, sealer, colour and clear. Not each one. All of them.
WHY MODERN PAINT IS DIFFERENT FROM WHAT YOU LEARNED ONOld acrylic lacquer and enamel were forgiving because they were low solids and they dried by evaporation. You could load them on and the solvent found its way out eventually. Polyurethane does not dry, it cures. It cross-links from the surface down, and once the top has gone off, anything still underneath is trapped. A heavy film skins over before its own solvent has left, and everything that goes wrong after that — pop, die-back, soft film, cracking two years later — is that trapped solvent. Modern 2K is a high-solids, low-build system. It is built to go on thin. Less is better, and less is not a compromise.

01THE STACK — WHERE EVERY MICRON GOES

Clearcoat
40-70 µm
Two coats. A third coat does not add gloss, it adds microns and takes the film past its limit.
Basecoat
15-25 µm
Colour only. Metallics over 25 µm go dark and mottle — the flake cannot orient in a thick film.
Sealer / wet-on-wet
25-35 µm
Thin by design. Over-applying a sealer is the most common hidden cause of pop under colour.
2K primer surfacer
50-80 µm
The filling layer. 80 µm is the ceiling. A third coat to chase a low spot is the wrong fix.
Body filler
SHAPED BACK — NOT FILM BUILD
Over epoxy, never bare metal, never over etch. Shape it back — the filler you sand off is not film build.
Epoxy primer
40-60 µm
Bare metal only. Thin and even — it is an adhesion and corrosion layer, not a filler.
SUBSTRATE
BARE STEEL / PREPARED PANEL — NOT FILM BUILD
Everything above is measured from here. A DFT gauge on bare steel reads zero; on e-coat, subtract the e-coat reading first.
0
15
30
45
60
75
90 µm

Built the way it should be, a full repair from bare metal lands around 170-260 µm. That leaves headroom under 300. It is only when a layer is doubled — a third primer coat, a third clear coat, colour laid on to hide instead of to cover — that the stack goes over.

02THE THREE WAYS A JOB GETS OVERLOADED

1 · ONE MORE COATAlmost always to fix something the previous coat should have fixed. A third clear coat does not add gloss — gloss comes from flow and flash, not from thickness. A third primer coat to bury a low spot adds 25-40 µm and buries nothing: the low spot is still there under more material.
2 · TOO MUCH IN THE COATGun held too close, moved too slowly, or pressure too low. A wet coat that looks beautiful going on is usually 50% over. Check the gun setup on the TDS and check it against the gun, not against memory.
3 · NOT ENOUGH FLASHThe one nobody counts as overload, and the one that does the most damage. Coat two on top of coat one before coat one has released its solvent is not two coats — it is one thick coat with solvent locked in the middle.
FLASH-OFF IS NOT A DELAY, IT IS A PROCESS STEPThe flash time on the sheet is how long that film needs to let its solvent go at 20 °C. It is not padding and it is not a suggestion. Cold weather makes it longer, not shorter. The flash before the bake is the most skipped step in the trade and the single most common cause of solvent pop — the oven drives the remaining solvent to the surface faster than the film can release it, and it blows through.

03WHAT OVERLOAD ACTUALLY DOES

WHAT YOU SEEWHENWHAT HAPPENED
Solvent popafter the bakeSolvent trapped under a skinned film boiled out and blew craters through it. Film too heavy, or flashed too short before the bake.
Die-backhours to days afterGloss falls away as solvent keeps leaving and the film shrinks. Almost always a heavy clear or a heavy coat underneath it.
Soft filmdays to weeksNever fully cured. Marks under a fingernail, water-spots, holds a print. A thick film cannot cross-link through its depth.
Cracking / crazingmonths to yearsTotal build too high and too rigid over a flexible or thick substrate. The film cannot move with the panel.
Dark or mottled metallicimmediatelyBasecoat over 25 µm. The flake cannot orient in a thick wet film, so it sits at random and reads dark and patchy.
Edge mapping / ringingafter the bakeSolvent from a heavy topcoat re-softened a heavy underlayer at the feather edge.
Shrinkage over fillerweeksSand scratches and filler edges telegraph through as the over-thick primer above them keeps shrinking.

04MEASURE IT

IF THE PANEL IS ALREADY OVERDo not put more on top hoping to level it. Sand the build back into range before you go further. If the existing finish is already at or past 300 µm before you have added anything, that panel needs stripping, not another system over the top. Nothing you spray will fix a film that cannot get its solvent out.

05EVERY GERMA-TECH PRODUCT — BUILD, MAXIMUM, FLASH

Taken straight from the current technical data sheets. Where a sheet has no maximum stated, treat the top of the build range as the maximum.

PRIMERS & UNDERCOATS

CODEPRODUCTCOATSFILM BUILDMAXIMUMFLASH BETWEEN COATS
GP13901K PLASTIC PRIMER (GREY) GP1390Wet Spray 2.5 coats MAX (1 light tack coat + 2 solid coats)1-2 µm2 µm (2.5 coats (1 light tack coat + 2 solid coats) at 1-2 µm is maximum)10 min at 20 °C between coats (allow extra time in colder conditions)
GP35011K PRIMER SURFACER2.5 coats (1 light tack coat + 2 solid coats)40-60 µm totalAt 20 °C, 5-10 minutes
GP34012K EPOXY PRIMER2.5 coats (1 light tack coat + 2 solid coats)40-60 µm totalAt 20 °C 5-10 minutes between coats
GP33252K PLASTIC PRIMER (GREY) GP3325Wet Spray 2.5 coats MAX (1 light tack coat + 2 solid coats)10-20 µm20 µm (2.5 coats (1 light tack coat + 2 solid coats) at 10-20 µm is maximum)
GP46482K PRIMER HI-FILL SURFACER - NO REDUCER2.5 coats (1 light tack coat + 2 solid coats). First coat - 1/2 coat…50 - 80 µm total80 µmAt 23 °C 3-6 minutes between coats (adjust flash off longer or shorter based on climate conditions)
GP31012K PRIMER SURFACER - HI FILL2.5 coats (1 light tack coat + 2 solid coats)50 - 80 µm total80 µmAt 23 °C 5-7 minutes between coats (flash off longer in cold climate)
GP-AI-301AUTO INDUSTRIAL 2K PRIMER HI FILL SURFACERApply two even coats (2.5 coats (1 light tack coat + 2 solid coats)…40-80 µm (2 coats preferred at build 40-80UM)Standard 80 µm, can build to 150 µm10 minutes flash off between coats, apply second coat once touch dry but still tacky
GP-AI-201AUTO INDUSTRIAL EPOXY PRIMER / EPOXY HIGH…2.5 coats (1 light tack coat + 2 solid coats) (GP-AI-201 TDS);…Wet-on-wet 1-2 coats, 40-80 µm · sanding build 2 coats, 40-100 µm100 µm of this productAt 20 °C 15-20 minutes between coats (GP-AI-201 TDS); Allow 5-20 minutes flash off between coats at 25 °C,…
GP3401FFAST DRY EPOXY PRIMER2.5 coats (1 light tack coat + 2 solid coats)40-60 µm total60 µm of this productAt 20 °C 5-10 minutes between coats
GP3201MULTI 2K PRIMER PLUS (3:1) - SPEED PRIMER…HI FILL: 2.5 coats maximum (tack coat followed by 2 solid coats) |…HI FILL 50-80 µm | WET ON WET 25-35 µm80 µm (Hi Fill)Speed Spot Repairs: 1 minute or no flash time | Standard Repair: 2 - 3 minutes (adjust up in cooler…
GP3301PLASTIC PRIMER (1K, TRANSPARENT)1 coat1 - 2 µm2 µmAt 20 °C 5-10 minutes between coats

COLOUR & TOPCOATS

CODEPRODUCTCOATSFILM BUILDMAXIMUMFLASH BETWEEN COATS
GPFEXC100ACRYLIC BINDER2.5 coats (1 light tack coat + 2 solid coats)40 µm totalAt 20 °C, 2-3 minutes between coats
GP AUTO 2K COLOUR2.5 coats (1 light tack coat + 2 solid coats)40-60 µm total60 µm of this productAt 20 °C, 5-10 minutes between coats
GP-1K BASECOAT COLORS (SOLVENT)2.5 coats (1 light tack coat + 2 solid coats)15-25 µm totalthe metallic paint film should not be thicker than 25 µmAt 23 °C, 5-10 minutes between coats
NT FLEET LINE 2K COLOUR2 Coats40-60 µm total60 µm of this productAt 20 °C, 5-10 minutes between coats
SHOWELL SH 1K WATERBORNE BASECOATSOLID: 1. Apply one wet coat firstly at a gun distance of 10-15 cm.…15 +/- µmSolid: blow off or bake till the surface is dry between coats (no time stated). Metallic: 2-3 minutes after…

CLEARCOATS

CODEPRODUCTCOATSFILM BUILDMAXIMUMFLASH BETWEEN COATS
GP4301FAST DRYING CLEAR COAT (AIR DRY CLEAR) 4:12.5 coats (1 light tack coat + 2 solid coats)40-60 µm total60 µm of this productContinuous wet-spray without flash off time between coats is better for paint leveling
GP899KGP899 SUPER HS GLAMOUR CLEAR2.5 coats (1 light tack coat + 2 solid coats) — or 2 solid coats40-60 µm total60 µm of this product5-10 minutes at 20 °C
GP4410HIGH VELOCITY CLEAR COAT2 Coats40 µm totalAt 20 °C, NO FLASH OFF TIME between coats
GP4101HS HIGH SOLID CLEAR COAT2.5 coats (1 light tack coat + 2 solid coats)50-70 µm total70 µm of this product5-10 minutes at 20 °C
GP4411MIRROR EFFECT CLEAR COAT2.5 coats (1 light tack coat + 2 solid coats)40-60 µm total60 µm of this product5-10 minutes at 20 °C
GP4201MS MEDIUM SOLID CLEAR COAT - SUPER HIGH…2.5 coats (1 light tack coat + 2 solid coats)40-60 µm total60 µm of this product5-10 minutes at 20 °C
SNAP CLEAR COAT2 Wet Coats (max 2 coats)40-60 µm totalAt 20 °C, 2-3 minutes between two wet coats (max 2 coats)
GP4403SUPER HS PREMIUM CLEAR COAT2.5 coats (1 light tack coat + 2 solid coats)50-70 µm total70 µm of this product5-10 minutes at 20 °C

ANCILLARY

CODEPRODUCTCOATSFILM BUILDMAXIMUMFLASH BETWEEN COATS
GPFUNC102K TEXTURE COAT1-3 Coatstotal 150-450 µm60 minutes at 20 ˚C
GA117RUBBERISED UNDERCOATING1LT sheet: spray a thin layer, repeat this process 3 times at an…1LT sheet: When the undercoating thickness reaches 2mm, better noise deadening effect…1LT sheet: at least 10 minutes between sprays at normal temperature

Issued by Terry Livingstone Trading Pty Ltd as trustee for the Terry Livingstone Trading Trust, trading as Ampro Australia. This guide is the document referenced as the "Germatech Coating Thickness Guide" on Germa-Tech technical data sheets. Figures are taken from the current TDS for each product and change with them. All times and film builds are quoted at 20 °C and 50% relative humidity unless stated otherwise. Read the Safety Data Sheet before use.

GERMA-TECH · AMPRO AUSTRALIA · WESTMEADOWS VIC 3049 · germatech.com.au · support@amproaustralia.com